Microstructure and properties of p-type (Bi0.25Sb0.75)2Te3 fabricated by spark plasma sintering
来源期刊:中国有色金属学报(英文版)2007年增刊第1期(Part ⅡB)
论文作者:王富强 陈晖 王忠 成艳 褚颖 朱磊 简旭宇
文章页码:1010 - 1013
Key words:(Bi0.25Sb0.75)2Te3; thermoelectric material; spark plasma sintering(SPS); sintering temperature
Abstract: P-type thermoelectric material (Bi0.25Sb0.75)2Te3 was sintered by spark plasma sintering(SPS) process in the temperature range of 320-420 ℃. The microstructures of sintered materials were found to be well aligned, particularly when sintered at lower sintering temperatures. The electrical conductivity of the material became larger as the sintering temperature increased. The Seebeck coefficient showed a general decreasing tendency with an increase in sintering temperature. In terms of the power factor, the optimum sintering temperature was found to be 380 ℃ for a maximum value of around 2.6 mW/K.